Heat Treatment
Heat-treating is performed to change certain characteristics of metals and alloys in order to make them more suitable for a particular kind of application. In general, heat treatment is the term for any process employed, by either heating or cooling, to change the physical properties of a metal. The goal of heat treatment is to change the structure of the material to a form, which is known to have the desired
properties. The treatments induce phase transformations that greatly influence mechanical properties such
as strength, hardness, ductility, toughness, and wear resistance of the alloys. The large number of service requirements and amount of alloys available make for a considerable amount of heat-treating operations.
Heat Treatment of Carbon Steels and Carbon Alloy Steels
Carbon steels and carbon alloy steels can be heat treated for the purpose of improving properties such as hardness, tensile and yield strength. The desired results are accomplished by heating in temperature ranges where a phase or combinations of phases are stable, and/or heating or cooling between temperature ranges
in which different phases are stable.
The structure of steel is composed of two variables:
1. Grain Structure - The arrangement of atoms in a metal.
2. Grain Size - The size of the individual crystals of metal. Large grain size is generally associated with low strength, hardness, and ductility.
After being formed, the material is usually quenched and tempered to produce a martensitic structure that produces the most sought after mechanical properties in steel fasteners. Martensite is formed by rapid cooling or quenching from austenizing temperatures using a quenching medium, such as oil, water or air, that will transfer heat away from the hot parts at a sufficient rate. The quenched martensitic structure,
which is hard but brittle, is then tempered in order to increase the ductility and decrease the hardness to specified levels. During the quenching treatment, it is impossible to cool the specimen at a uniform rate throughout. The surface of the specimen will always cool more rapidly than the interior regions.
7
Therefore, the austenite will transform over a range of temperatures, yielding a possible variation of microstructure and properties with position within the material.
The successful heat treatment of steels to produce a predominantly martensitic microstructure throughout the cross section depends mainly on three factors:
1. the composition of the alloy
2. the type and character of the quenching medium
3. the size and shape of the specimen
Hardenability
The influence of alloy composition on the ability of a steel alloy to transform to martensite for a particular quenching treatment is related to a parameter called hardenability. For every different steel alloy there is a specific relationship between their mechanical properties and their cooling rate. Hardenability is not
“hardness” which is a resistance to indentation; rather, hardness measurements are utilized to determine the extent of a martensitic transformation in the interior of the material. A steel alloy that has a high
hardenability is one that hardens, or forms martensite, not only at the surface but also to a large degree throughout the entire interior. In other words, hardenability is a measure of the depth to which a specific alloy may be hardened.
The following elements have known effects on the properties of steel:
Carbon ( C ): Primary alloying element: Principle hardening element: Essential for the formation of martensite during hardening
Manganese ( Mn ): Increases strength and hardness: Increases hardenability
Phosphorus ( P ): Considered an impurity, can cause brittleness at low temperatures Sulfur ( S ): Considered an impurity, can lower tensile strength at high temperatures: Improves machinability in free machining steels
Silicon ( Si ): Deoxidizer
Nickel ( Ni ): Improves toughness: Simplifies heat-treating: Increases hardenability: Decreases distortion: Improves corrosion resistance
Chromium ( Cr ): Improves hardenability: Provides wear and abrasion resistance: Improves corrosion resistance
Molybdenum ( Mo ): Improves hardenability: Non-oxidizing
Boron ( B ): Trace amounts increase hardenability: Promotes formability
Aluminum ( Al ): Controls grain size: Deoxidizer
Tempering
In the as-quenched state, martensite, in addition to being very hard, is extremely brittle and cannot be used for most applications. Also, any internal stresses that may have been introduced during quenching have a weakening effect.
If the steel has been fully hardened by being quenched from above its critical temperature, tempering can
be used to enhance the ductility and toughness of martensite and relieve the internal stresses. In tempering, the steel is reheated to a specific temperature below its critical temperature for a certain period of time and then cooled at a prescribed rate.
The following example will demonstrate the effectiveness of tempering:
ASTM A193 Grade B7, SAE J429 Grade 8 and ASTM A574 Socket Head Cap Screws are all made from alloy steels. In fact some alloy steel grades can be used to manufacture any of the three final products:
such as 4140 and 4142 alloy steel. The final mechanical properties are the following: ASTM A193 B7
• Tensile Strength: 125,000 PSI minimum (2-1/2-inch and under)
• Yield Strength: 105,000 PSI minimum (2-1/2-inch and under)
• Hardness: HRC 35 Maximum
SAE J429 Grade 8
• Tensile Strength: 150,000 PSI minimum
8
• Proof Strength: 120,000 PSI
• Yield Strength: 130,000 PSI minimum
• Hardness: HRC 33-39
ASTM A574 Socket Head Cap Screw
• Tensile Strength: 180,000 PSI minimum (through ½”), 170,000 PSI minimum (above ½”)
• Proof Strength: 140,000 PSI (through ½”), 135,000 PSI (above ½”)
• Yield Strength: 153,000 PSI minimum
• Hardness: HRC 39-45 (through ½”), HRC 37-45 (above ½”)
The initial heat-treating process is relatively the same for all three products. The parts are heat treated until fully austenitized. The parts are then quenched and tempered in a liquid (oil). This final tempering temperature is what will dictate our final product. The following are the minimum tempering temperatures
for each specification:
• ASTM A193 B7: 1150°F
• SAE J429 Grade 8: 800°F
• ASTM A574: 650°F
As can be seen by the results, a lower tempering temperature will produce a harder and higher tensile strength part for these alloy steels. However, the lower tempering temperatures will also mean lower service conditions, ductility, impact strength and possible fatigue life. For example a B7 has a high- temperature limitation of approximately 750-800°F. The socket head cap screws and grade 8’s have a limitation of approximately 400-500°F.